PC; VITA Zahnfabrik, Bad Sackingen, Germany). Forty-five specimens of each material were tested. Micro-hardness was measured at baseline, after 7 days and after 28 days. The data were analyzed. The micro-hardness of each material varied significantly after immersion in Coca-Cola. The nanohybrid composite had a high initial micro-hardness and the greatest percentage loss after acid exposure. The hybrid ceramic and the resin nano ceramic had similar percentage losses of micro-hardness values even if the second material had higher initial values. The zirconia-reinforced lithium silicate glass ceramic had the highest baseline values and the lowest percentage loss of micro-hardness. The different CAD/CAM materials presented different micro-hardness values before and after acid exposure.
No takes yet. Share an insight, caveat, or question.
Colombo et al. (2019) studied this question.
Synapse has enriched 5 closely related papers on similar clinical questions. Consider them for comparative context: