Single phase powders of BaTi2O5 and Ba6Ti17O40 were made by a sol-gel method with final heating at 1100–1200°C. Ceramic samples were prepared and fired at temperatures in the range 1100–1300°C. Both sets were highly insulating, with conductivities of, e.g., 10−6–10−7Scm−1 at 600°C and activation energies for conduction in the range 1.75–1.86eV. BaTi2O5 compositions are ferroelectric with a permittivity maximum dependent on firing conditions: εmax′=122 at 450°C on firing at 1100°C; and εmax′=130 at 475°C on firing at 1225°C. Ba6Ti17O40 is a dielectric with ε′∼57–55 over the range 40–400°C.
No takes yet. Share an insight, caveat, or question.
Beltrán‐Mir et al. (2005) studied this question.