Progress in building construction requires more durable concrete with higher strength. Polymer and water reducer liquids can improve concrete strength and durability. This research aims to improve the mechanical properties of polymer-modified concrete by using anti-slip sand and silica fume to achieve more durable concrete against sulfate attack and higher mechanical properties. The study shows an increase in compressive strength from 25.7 MPa for reference mix to 45.5 MPa using 15% silica fume and 30% Anti-slip sand; tensile strength increased from 2.72 to 4.4 MPa. Flexural strength also increased, and durability to sulfate attack also increased. The study includes the increment of durability against freezing-thawing cycles for different mixes.