Three different contact schemes Al–Si, Al/Ti–Si, and Al/TiN/Ti–Si have been studied for their electrical characteristics and thermal stability on shallow n+p-junctions. Contact resistance and leakage current measurements indicate that the Al/Ti structure remains stable up to 450 °C and the Al/TiN/Ti structure up to 500 °C for 15 min, whereas Al–Si contacts degrade already at 400 °C. The stability of the Al/Ti contacts is limited by the thin film reaction between Al and Ti while the failure of the Al/TiN/Ti structure is attributed to local defects such as pinholes in the TiN barrier.
No takes yet. Share an insight, caveat, or question.
Suni et al. (1985) studied this question.
Synapse has enriched 5 related papers. Consider them for comparative context: