Answers are grounded in this paper and cite their sources.
The Hall coefficient of titanium has been measured over a temperature range from 350°K to 1100°K. The coefficient is −2.0×10−11m3/coulomb near room temperature, reverses sign at (675±30)°K, and increases to a value of +3.5×10−11m3/coulomb at 1100°K. The measurements were made on titanium samples which had a purity of 99.99%. The samples were heated by direct current, and the temperatures were determined indirectly from the resistivity measurements which were made with each Hall measurement. The resistivity is 0.48 microhm m at 350°K. It increases to a maximum of 1.76 microhm m at the crystal transition temperature.
No takes yet. Share an insight, caveat, or question.
Georgiana W. Scovil (1956) studied this question.
Synapse has enriched 10 related papers. Consider them for comparative context: