Answers are grounded in this paper and cite their sources.
Films of Ni-7 at% V, Pt, Pd, and , each approximately 100 nm thick, were magnetron-deposited and interposed between about 250 nm thick copper overlayers and single-crystalline substrates. The samples were then annealed in vacuum up to C. The performance of the metal and the tantalum-silicon-nitride films as diffusion barriers for in-diffusion of Cu and out-diffusion of Bi and Te was evaluated by 2.0 MeV backscattering spectrometry and x-ray diffraction. The Ni-7 at% V, Pd and Pt films all fail to prevent interdiffusion of Cu and after a few hours of annealing at C. However, the barrier preserves the integrity of the contact after C for 50 h and C for 1 h anneals. These results confirm the superior characteristics of the metal-silicon-nitride films as diffusion barriers.
No takes yet. Share an insight, caveat, or question.
Kacsich et al. (1998) studied this question.
Synapse has enriched 10 related papers. Consider them for comparative context: