Answers are grounded in this paper and cite their sources.
First magnetocrystalline anisotropy constants K1∞ of 3.6, 6.7, 8.8, and 12.4 wt% silicon in iron alloys have been measured at 77°K and 297°K by determining the torque exerted on {100} single-crystal disks in uniform magnetic fields. The following results on disordered alloys have been obtained: Composition (wt%Si)Temperature (∘K)K1∞×103(erg cm−3)3.677430±10297360±106.777290±10297205±108.877245±10297165±1012.477120±529778±5 The measurements of this investigation are compared with the previously known studies. The agreement, where an overlap occurs, is satisfactory.
No takes yet. Share an insight, caveat, or question.
Arajs et al. (1961) studied this question.