Answers are grounded in this paper and cite their sources.
The Hall mobility and carrier concentration have been measured on low-resistivity ZnSe epitaxial films in the temperature range of 77–300 K. Both undoped and indium doped materials were studied. Resistivities of the as-grown films varied from 10−1 to 105 Ω cm. Electron mobility was of the order of 10–200 cm2 V−1 s−1 and was limited by ionized-impurity scattering. Analysis of the temperature dependence of the carrier concentration and Hall mobility indicated that the n-type films were heavily compensated having acceptor concentrations NA≳1018 cm−3. It was found that the acceptor and donor concentrations were essentially independent of Zn/Se pressure ratio present during growth.
No takes yet. Share an insight, caveat, or question.
Leigh et al. (1982) studied this question.
Synapse has enriched 10 related papers. Consider them for comparative context: