Answers are grounded in this paper and cite their sources.
Interfacial microstructures of Pd/Ge/Ti/Au ohmic contact to n-type GaAs have been investigated using cross-sectional transmission electron microscopy, and the results are used to interpret the electrical properties. Annealing at 300 °C yields a contact resistance of 0.62 Ω mm and the layer structure is changed to GaAs/PdGe/Au4Ti/TiO. The ohmic contact is formed through a solid phase regrowth of GaAs heavily doped with Ge below the PdGe layer. At 380 °C, the lowest contact resistance of 0.43 Ω mm is obtained. The layer structure is changed to GaAs/(Ge–Ti)/PdGe/TiO. Spikes composed of Au and AuGa are found at the grain boundaries of the PdGe compound. The formation of AuGa at 380 °C reduces the contact resistance through the creation of more Ga vacancies at the interface of GaAs/PdGe, and the incorporation of elemental Ge.
No takes yet. Share an insight, caveat, or question.
Kwak et al. (1996) studied this question.
Synapse has enriched 10 related papers. Consider them for comparative context: