Answers are grounded in this paper and cite their sources.
Bi-Sr-Ca-Cu-O superconducting fibers were prepared by the sol-get method. Gel fibers of 0.01–1 mm diameter were directly drawn from a homogeneous viscous sol which was prepared from an aqueous solution of metal acetates containing acetic acid and tartaric acid. Ceramic fibers with the high-T c phase as the main phase were obtained by heating the gel fibers derived from the sol of molar composition of Bi:Pb:Sr:Ca:Cu=1.85:0.35:1.9:2.0:3.1 to 835°C at a slow rate of 0.33°C/min and keeping them there for 40 h. The fiber showed diamagnetism below 110 K and zero electrical resistance at 98 K.
No takes yet. Share an insight, caveat, or question.
Zhuang et al. (1989) studied this question.
Synapse has enriched 10 related papers. Consider them for comparative context: