Answers are grounded in this paper and cite their sources.
The glass composition, MgO 11.5%, Al2O3 21.4%, SiO2 60.5% and TiO2 6.4% (by weight), was crystallised, at different temperatures ranging from 825 to 1225° under controlled conditions. The crystal phases were detected by X-ray method and the modulus of rupture, thermal expansion and density of the crystallised samples were measured. All the three properties increased to a maximum with increasing crystallisation temperature. Higher density and thermal expansion of the crystal phases have been shown to produce compressive stress on glass and, as a result, the strength increases to a maximum of 5,500 kg/cm2, compared to 1,700 kg/cm2 for uncrystallised glass. The relations between stress, thermal expansion and density have been discussed quantitatively.
No takes yet. Share an insight, caveat, or question.
Kumar et al. (1963) studied this question.